无锡20G高压锅炉管化学成分及材质分析表-洋利特钢管
标准 |
牌号 |
化学成分(%) |
C |
Si |
Mn |
P |
S |
Cr |
Mo |
Cu |
Ni |
V |
Al |
W |
Ti |
Nb |
N |
GB3087 |
10 |
0.07~0.13 |
0.17~0.37 |
0.38~0.65 |
≤0.030 |
≤0.030 |
0.3~0.65 |
/ |
≤0.25 |
≤0.30 |
/ |
/ |
|
|
|
|
20 |
0.17~0.23 |
0.17~0.37 |
0.38~0.65 |
≤0.030 |
≤0.030 |
0.3~0.65 |
/ |
≤0.25 |
≤0.30 |
/ |
/ |
|
|
|
|
|
GB5310 |
20G |
0.17~0.24 |
0.17~0.37 |
0.35~0.65 |
≤0.030 |
≤0.030 |
≤0.25 |
≤0.15 |
≤0.20 |
≤0.25 |
≤0.08 |
|
|
|
|
|
20MnG |
0.17~0.24 |
0.17~0.37 |
0.70~1.00 |
≤0.030 |
≤0.030 |
≤0.25 |
≤0.15 |
≤0.20 |
≤0.25 |
≤0.08 |
|
|
|
|
|
|
25MnG |
0.18~0.24 |
0.17~0.37 |
0.80~1.10 |
≤0.030 |
≤0.030 |
≤0.25 |
≤0.15 |
≤0.20 |
≤0.25 |
≤0.08 |
|
|
|
|
|
|
15CrMo |
0.12~0.18 |
0.17~0.37 |
0.40~0.70 |
≤0.030 |
≤0.030 |
0.80~1.10 |
0.40~0.55 |
≤0.20 |
≤0.30 |
|
|
|
|
|
|
|
12Cr2MoG |
0.08~0.15 |
≤0.50 |
0.40~0.70 |
≤0.030 |
≤0.030 |
2.00~2.50 |
0.90~1.20 |
≤0.20 |
≤0.30 |
|
|
|
|
|
|
|
12Cr1MoV |
0.08~0.15 |
0.17~0.37 |
0.40~0.70 |
≤0.030 |
≤0.030 |
0.90~1.20 |
0.25~0.35 |
≤0.20 |
≤0.30 |
0.15~0.30 |
|
|
|
|
|
|
12Cr2MoWVTiB |
0.08~0.15 |
0.45~0.75 |
0.45~0.65 |
≤0.030 |
≤0.030 |
1.60~2.10 |
0.50~0.65 |
≤0.20 |
≤0.30 |
0.28~0.42 |
|
0.30~0.55 |
0.08~0.15 |
B 0.002~0.008 |
|
|
10Cr9Mo1VNb |
0.08~0.12 |
0.20~0.50 |
0.30~0.60 |
≤0.020 |
≤0.010 |
8.00~9.50 |
0.85~1.05 |
≤0.20 |
≤0.40 |
0.18~0.25 |
≤0.015 |
|
|
0.06~0.10 |
0.03~0.07 |
|
ASME SA210 |
SA210A-1 |
0.13~0.19 |
≥0.1 |
0.45~0.65 |
≤0.030 |
≤0.030 |
|
|
|
|
|
|
|
|
|
|
SA210C |
0.18~0.24 |
≥0.1 |
0.80~1.10 |
≤0.030 |
≤0.030 |
|
|
|
|
|
|
|
|
|
|
|
ASME SA213 |
SA213 T11 |
0.05~0.15 |
0.50~1.0 |
0.30~0.60 |
≤0.030 |
≤0.030 |
1.00~1.50 |
0.50~1.00 |
|
|
|
|
|
|
|
|
SA213 T12 |
0.05~0.15 |
≤0.50 |
0.30~0.61 |
≤0.030 |
≤0.030 |
0.80~1.25 |
0.44~0.65 |
|
|
|
|
|
|
|
|
|
SA213 T22 |
0.05~0.15 |
≤0.50 |
0.30~0.60 |
≤0.030 |
≤0.010 |
1.90~2.60 |
0.87~1.13 |
|
|
|
|
|
|
|
|
|
SA213 T23 |
0.04~0.10 |
≤0.50 |
0.10~0.60 |
≤0.030 |
≤0.030 |
1.90~2.60 |
0.05~0.30 |
|
|
|
≤0.030 |
1.45~1.75 |
B 0.0005~0.006 |
0.02~0.08 |
≤0.040 |
|
SA213 T91 |
0.08~0.12 |
0.20~0.50 |
0.30~0.60 |
≤0.020 |
≤0.010 |
8.00~9.50 |
0.85~1.05 |
|
≤0.40 |
0.18~0.25 |
≤0.015 |
|
|
0.06~0.10 |
0.03~0.07 |
|
SA213 T92 |
0.07~0.13 |
≤0.50 |
0.30~0.60 |
≤0.020 |
≤0.010 |
8.50~9.50 |
0.30~0.60 |
|
≤0.40 |
0.15~0.25 |
≤0.015 |
1.50~2.00 |
B 0.001~0.006 |
0.04~0.09 |
0.03~0.07 |
|
DIN 17175 |
ST45.8/<, SPAN style="FONT-WEIGHT: bold; FONT-SIZE: 9pt; COLOR: rgb(0,0,0); FONT-FAMILY: '宋体'">Ⅲ |
≤0.21 |
0.10~0.35 |
0.40~1.20 |
≤0.040 |
≤0.040 |
|
|
|
|
|
|
|
|
|
|
15Mo3 |
0.12~0.20 |
0.10~0.35 |
0.40~0.80 |
≤0.035 |
≤0.035 |
|
0.25~0.35 |
|
|
|
|
|
|
|
|
|
13CrMo44 |
0.10~0.18 |
0.10~0.35 |
0.40~0.70 |
≤0.035 |
≤0.035 |
0.70~1.10 |
0.45~0.65 |
|
|
|
|
|
|
|
|
|
10CrMo910 |
0.08~0.15 |
≤0.50 |
0.30~0.70 |
≤0.025 |
≤0.020 |
2.00~2.50 |
0.90~1.10 |
≤0.30 |
≤0.30 |
|
≤0.015 |
|
|
|
|
|
20高压锅炉管是属于优质碳素结构钢(GB/T699-1999),优质碳素结构钢是依靠调整含碳(C)量来改善钢的力学性能,因此,根据含碳量的高低,此类钢又可分为:
低碳钢--含碳量一般小于0.25%,如10、20钢等;
中碳钢--含碳量一般在0.25~0.60%之间,如35、45钢等;
高碳钢--含碳量一般大于0.60%。此类钢一般不用于制造钢管。
实际上,他们之间的含碳量并没有明显的界限。
此类钢产量较大,用途较广,一般多轧(锻)制成圆、方、扁等型材、板材和无缝钢管。主要用于制造一般结构及机械结构零、部件以及建筑结构件和输送流体用管道。根据使用要求,有时需热处理(正火或调质)后使用。
高压锅炉用无缝钢管(GB5310-1995)是用于制造高压及其以上压力的水管锅炉受热面用的优质碳素钢、合金钢和不锈耐热钢无缝钢管。